Pulse Opaque Firing Guide

Opaque Firings:

Spatulate the Pulse paste opaque before applying. Use the Pulse paste opaque liquid for dilution, if necessary.

Apply a full even layer of paste opaque to the framework and modify with intensive opaques according to the desired chroma intensity.

In the case of non-precious alloys, it is recommended to use powder opaque for the first opaque firing/ wash for the best results.

Pulse Press-To-Metal® (precious alloys)
 
Start Temp
Closing Time
Start
Vacuum
Temp. Increase
Final Temp
Hold
Time
Cooling
Time
Degassing
400 C
1 min.
*
55-80C
*
*
0
1st + 2nd Opaque Firing
400 C
8 min.
400 C
55C
950 C
1 min
0
Pulse Press-To-Metal® (non-precious alloys)
 
Start Temp
Closing Time
Start
Vacuum
Temp. Increase
Final Temp
Hold
Time
Cooling
Time
Degassing
400 C
1 min.
*
80C
*
*
0
Powder Opaque Firing 400 C
6 min.
400 C
55C
980 C
1 min
0
Paste Opaque Firing
400 C
8 min.
400 C
55C
950 C
1 min
0

* Please refer to the Alloy Manufacturer